Two requirements shorten the material list faster than anything else: no magnetism, and no cobalt. For non-magnetic disc springs and washers, CuSn8 bronze is the option, accepting considerably lower strength and spring forces. For nuclear duty, Inconel X718 is virtually cobalt free, with excellent corrosion resistance and capability to 600 degrees C.
Most spring specifications are a negotiation between load, space and cost. These two are different. They are constraints on the material itself, which means the design has to move around them.
When magnetism is the constraint
Cold forming makes several otherwise attractive grades magnetic. X10 CrNi 18-8 and X7 CrNiAl 17-7 are corrosion resistant chromium nickel spring steels, but the cold forming process makes both magnetic. That is fine in most plant and a problem near sensors, imaging equipment, measurement instruments or anything with a magnetic field of its own.
There are two levels of answer. For low magnetisability stainless, X5 CrNiMo 17-12-2 (1.4401) austenitic stainless offers higher corrosion resistance and lower magnetisability than the chromium nickel grades. Where the requirement is genuinely anti-magnetic, CuSn8 bronze washers (2.1030) to DIN EN 1654 are the material used in the original SCHNORR family of non-magnetic serrated safety washers. It is a copper tin alloy that keeps its spring characteristics through cold forming.
What bronze costs you
This trade cannot be designed around after the fact, so it belongs in the first calculation: the strength values of CuSn8, and the spring forces that follow from them, are considerably lower than with standard material. A joint that was sized on carbon spring steel will not deliver the same clamp force in bronze. Either the stack grows, the number of fasteners grows, or the target force comes down.
When cobalt content is the constraint
For nuclear application springs, material provenance is part of the specification. Inconel X718 (2.4668) is virtually cobalt free, which is why it is often used in nuclear reactor technology, and it brings excellent corrosion resistance and suitability for high temperature applications up to 600 degrees C. Inconel X750 (2.4669) covers the same temperature range.
One behaviour to design for at that temperature: potential creeping under load, which can lead to a loss of installation height or a loss of force in the spring. Creep results from a combination of temperature, time and tension, so a long life preload application needs it accounted for.
Load washers follow the same logic
The load washer range carries the same two answers. Inconel X718 is offered as the virtually cobalt free option often used in nuclear reactor technology, and CuSn8 bronze as the anti-magnetic option, again with considerably lower strength values and resulting spring forces than standard material.
Documentation is part of the deliverable
In both cases the paperwork travels with the part. Certifications are published for download on schnorr.com, and where the requirement goes past the standard range, SCHNORR develops tailor made solutions in partnership with customers, further than DIN or EN, including special sizes.
A short specification note
State the constraint as a limit, not as a material. “No magnetic signature above X” or “cobalt free” leaves room for the right answer, where naming a grade sometimes rules out a better one. Then add force, installed height, space and temperature, and the shortlist writes itself.
- CuSn8 bronze (2.1030) to DIN EN 1654 is used in the original SCHNORR family of non-magnetic serrated safety washers.
- CuSn8 strength values and resulting spring forces are considerably lower than standard material.
- X10 CrNi 18-8 and X7 CrNiAl 17-7 are corrosion resistant but become magnetic through cold forming.
- X5 CrNiMo 17-12-2 (1.4401) offers higher corrosion resistance and lower magnetisability than those grades.
- Inconel X718 (2.4668) is virtually cobalt free and often used in nuclear reactor technology.
- Inconel X718 and X750 offer excellent corrosion resistance and suit temperatures up to 600 degrees C.
- Creeping under load from temperature, time and tension can cause loss of installation height or spring force.
- Load washers are also available in Inconel X718 and CuSn8 bronze.
Frequently asked questions
Which material is used for non-magnetic springs and washers?
CuSn8 bronze (2.1030) to DIN EN 1654, a copper tin alloy that retains its spring characteristics through cold forming. It is used in the original SCHNORR family of non-magnetic serrated safety washers.
What is the trade off with bronze springs?
Strength values and the resulting spring forces are considerably lower than with standard material, so the stack, the fastener count or the target force has to be adjusted.
Are stainless steel springs non-magnetic?
Not necessarily. X10 CrNi 18-8 and X7 CrNiAl 17-7 become magnetic through cold forming. X5 CrNiMo 17-12-2 offers lower magnetisability.
Which material suits nuclear applications?
Inconel X718 (2.4668) is virtually cobalt free and often used in nuclear reactor technology, with excellent corrosion resistance and suitability up to 600 degrees C.
Do high temperature springs lose force over time?